A

S355JR is a low-alloy, high-strength structural steel defined by the European standard EN 10025-2 (equivalent to the Chinese standard Q355B). It features a yield strength of ≥355 MPa and an impact energy of ≥27 J at -20°C, and is widely used in construction, machinery manufacturing, and shipbuilding.

Compositional characteristics: Carbon content is ≤0.22%; however, the presence of sulfur and phosphorus impurities (≤0.025%) increases the risk of hot cracking.

Strength and hardness: Tensile strength ranges from 470 to 630 MPa. When cutting thick plates (>40 mm), there is a high risk of thermal stress concentration.

S355JR has a higher yield strength than S235.

1. Cutting: For plates ≥40 mm thick or when working in low ambient temperatures, preheat the material to 100–150°C. Allow for slow cooling; do not use water quenching. Grind off any hardened edge layers before bending or welding.

2. Bending: Requires higher tonnage. The minimum inner bend radius should be ≥2t (along the rolling direction) and ≥2.5–3t (across the rolling direction). Springback is more pronounced than in S235. Avoid cold bending at temperatures below 5°C.

3. Machining: Use P-grade coated carbide tools and ensure an adequate supply of coolant. Remove hardened cut edges prior to machining to prevent tool chipping. The formation of long, continuous chips and built-up edges is common.